Schedule for 3+4" Doug Fir
« on: February 13, 2017, 12:22:48 PM »
I've been following this website for a while, but have never posted before this. I need to dry some 3-4" thick Douglas Fir in my Nyle Dehumid kilns to approx 15%. This is the schedule I am planning on working with and I am curious if anyone thinks i need to adjust this at all:

% MC   DB Temp (˚F)   WB Temp (˚F)   DEP
Above 30 %   115              96                    19
30 to 25 %   130              108            22
25 to 20 %   140              108            32
20 to 15 %   150              115            35
15 to Final %   160              115            45

Any thoughts?

Offline MichaelM

  • Forum Expert
  • Kiln Drying Enthusiest
  • *****
  • Posts: 98
    • View Profile
Re: Schedule for 3+4" Doug Fir
« Reply #1 on: February 14, 2017, 07:38:23 AM »
I would be inclined to use a 10F depression for the first few days to reduce the chance of checking.  Then at the end, use a 20-25F depression when the average MC is less than 20% to reduce the overdry and variability.  What you have will work, however.
Mike M.

 


Search


* Forum Experts

MichaelM MichaelM
Forum Expert
TimothyD TimothyD
Forum Expert
PhilM PhilM
Forum Expert
StavrosA StavrosA
Forum Expert

* Subscribe to Newsletter

* Upcoming Events

Sorry! There are no calendar events available at the moment.
\
SimplePortal 2.3.6 © 2008-2014, SimplePortal